skip to content
Solutions-In-Plastics.info » Products » Construction plastics » Comparison between properties
Comparison between properties
comparison between properties of construction plastics (68kB)
| Properties |
PE-HWU |
PP-DWU |
PVC |
PVDF |
PVC-C |
E-CTFE |
PPs |
| Density, g/cm³ |
0,955 |
0,915 |
1,44 |
1,78 |
1,54 |
1,68 |
0,95 |
| ISO 1183 |
| Yield stress, MPa |
22 |
32 |
58 |
55 |
53 |
31 |
32 |
| DIN EN ISO 527 |
| Elongation at yield, % |
9 |
8 |
3 |
8 |
4 |
4 |
8 |
| DIN EN ISO 527 |
| Elongation at break, % |
300 |
70 |
15 |
30 |
20 |
125 |
70 |
| DIN EN ISO 527 |
| Tensile modulus of elasticity, MPa |
800 |
1400 |
> 3000 |
1950 |
2300 |
1650 |
1300 |
| DIN EN ISO 527 |
| Impact strength, kJ/m² |
without break |
without break |
without break |
without break |
|
without break |
without break |
| DIN EN ISO 179 |
| Notched impact strength, kJ/m² |
12 |
7 |
4 |
12 |
7 |
|
6 |
| DIN EN ISO 179 |
| Ball indentation hardness, MPa |
40 |
70 |
130 |
120 |
100 |
56 |
70 |
| DIN EN ISO 2039-1 |
| Shore hardness (D) |
63 |
72 |
82 |
78 |
|
74 |
72 |
| ISO 868 |
| Mean coefficient of linear thermal expansion, K E-1 DIN 53752 |
1,8 × 10^-4 |
1,6 x 10^-4 |
0,8 x 10^-4 |
1,3x10^-4 |
0,21 x 10^-4 |
0,5 × 10^-4 |
1,6 x 10^-4 |
| Thermal conductivity, W/m * K |
0,38 |
0,22 |
0,159 |
0,14 |
0,021 |
0,15 |
0,22 |
| DIN 52612 |
| Fire behaviour |
normal |
normal |
|
|
certification |
|
|
| DIN 4102 |
inflam. |
inflam. |
B1 cert. |
B1 cert. |
FM 4910 |
low flam. |
B1 cert. |
| Dielectric strength, kV/mm |
47 |
52 |
39 |
25 |
|
14 |
22 |
| DIN IEC 60243-1 |
| Surface resistivity, Ohm |
10^14 |
10^14 |
10^13 |
10^13 |
|
10^15 |
10^14 |
| DIN IEC 60093 |
| Temperature range, °C |
-50 to 0+ 80 |
0 to +100 |
0 to +60 |
-30 to + 140 |
-40 to +100 |
-40 to +150 |
0 to +100 |
| Physiological safety in accordance with BfR |
yes |
yes |
no |
yes |
|
yes |
no |
This is a printed version of Solutions-In-Plastics.info of ERIKS nv.
© ERIKS nv, 2010.